Download data sheet

Select Language

Get datasheet by email
Close

Get datasheet by email

On this page

Mechanical Properties

Hide/Show specific columns Edit
Select columns to display
    Product type Thickness
    (mmin)
    Width
    (mmin)
    Length
    (mmin)
    Hardness 1)
    (HBW)
    Typical yield strength
    (MPaksi), not guaranteed
    Typical tensile strength
    (MPaksi), not guaranteed
    Typical Elongation A (%),
    not guaranteed
    Sheet 2.00 - 8.000.079 - 0.315 1000 - 175039.370 - 68.898 2000 - 1200078.740 - 472.440 360 - 440 1100159 1250181 10
    Plate 6.00 - 40.000.236 - 1.575 1800 - 320070.866 - 125.984 2000 - 1200078.740 - 472.440 360 - 440 1100159 1300188 10
    Plate 40.01 - 60.001.575 - 2.362 2000 - 250078.740 - 98.425 4000 - 9500157.480 - 374.015 360 - 440 1100159 1300188 10
    Plate 60.01 - 80.002.363 - 3.150 2000 - 250078.740 - 98.425 4000 - 6900157.480 - 271.653 360 - 440 1100159 1300188 10
    Compare parameters

    Select one parameter to compare

    Comparison

      1) Brinell Hardness is measured, according to EN ISO 6506-1 on milled surface 0.3-3.0mm below surface. Hardness value is being announced in the material certificate.
      Mechanical properties are tested in transverse direction and tabulated for information only and values are not shown in material certificate.

      Impact Properties

      Hide/Show specific columns Edit
      Select columns to display
        Product Longitudinal test, typical impact energy,
        Charpy V 10x10 mm test specimen 1)
        Raex® 400 sheet & plate 30 J / -40 °C22 ft-lbs / -40 °F
        Compare parameters

        Select one parameter to compare

        Comparison

          Product
          Raex® 400 sheet & plate
          Longitudinal test, typical impact energy,
          Charpy V 10x10 mm test specimen 1)
          30 J / -40 °C22 ft-lbs / -40 °F

          1) Impact testing according to EN ISO 148-1 is performed on thickness ≥6mm. The specific value corresponds to a full-size specimen. Impactvalues are tabulated for information only and value are not shown in material certificate.

          Chemical Composition

          Hide/Show specific columns Edit
          Select columns to display
            Product type C
            (max %)
            Si
            (max %)
            Mn
            (max %)
            P
            (max %)
            S
            (max %)
            Cr
            (max %)
            Ni
            (max %)
            Mo
            (max %)
            B
            (max %)
            Plate 0.23 0.80 1.70 0.025 0.015 1.50 1.00 0.50 0.005
            Sheet 0.16 0.50 1.60 0.025 0.010 1.20 1.00 0.25 0.005
            Compare parameters

            Select one parameter to compare

            Comparison

              The steel is grain refined.

              Carbon Equivalent CET(CEV)

              Hide/Show specific columns Edit
              Select columns to display
                Product type Sheet Plate Plate Plate
                Thickness (mmin) 2.00 - 8.000.079 - 0.315 6.00 - 20.000.236 - 0.787 20.01 - 32.000.788 - 1.260 32.01 - 80.001.260 - 3.150
                Typ CET(CEV) 1) 0.30 (0.48) 0.30 (0.44) 0.35 (0.53) 0.35 (0.57)
                Compare parameters

                Select one parameter to compare

                Comparison

                  1) The CEV value is being announced in the inspection certificate and the CET values are tabulated for information only.

                  CET and CEV formula

                  Tolerances

                  Thickness

                  Plates tolerances according to EN 10029 Class A, tighter tolerances upon agreement. Sheets tolerances according to EN 10051 Category A.

                  Length and Width

                  For plate tolerances according to EN 10029, tighter tolerances upon agreement. Sheets tolerances according to EN 10051.

                  Shape

                  Tolerances according to EN 10029 for plate and according to EN 10051 for sheet.

                  Flatness

                  For plate and sheet the flatness deviation is max 6 mm/m.

                  Surface Properties

                  According to EN 10163-2 Class A, Subclass 3.

                  Bending

                  Minimum inner bending radii for a 90° bend, t ≤ 20 mm are:

                  Sheets and plates, 3 x t (transverse) and 4 x t (longitudinal).

                  Delivery Conditions

                  The delivery condition is quenched. Sheets are available in as rolled surface condition with mill edge. Plates are available in as-rolled or shopprimed surface condition. Delivery requirements can be found in SSAB´s brochure at www.raexsteel.com.

                  Fabrication and Other Recommendations

                  Welding, bending and machining recommendations can be found in brochures at www.raexsteel.com or consult Tech Support.

                  Raex® is not intended for further heat treatment. Mechanical properties are achieved by quenching. The properties of the delivery condition cannot be retained after exposure to temperatures in excess of 250°C.

                  Appropriate health and safety precautions must be taken when welding, cutting, grinding or otherwise working on this product. Grinding, especially of primer coated plates, may produce dust with a high particle concentration.